How to Improve the Wet Rubbing Fastness of Dye-Sub Fabric
1. Strengthen the pre-treatment, especially the process of boil-out bleaching Using a mild non-caustic oxygen bleaching process(such as oxygen bleach accelerator + H2O2) to avoid the wet rubbing fastness affected by fiber brittleness, the rough surface of the fabric and the large friction coefficient of the fabric yarn surface in the process of oxygen bleaching. Strict control of water hardness to prevent the formation of surface lakes, causing the rough feel of the dye, increasing the friction coefficient and decreasing the wet rubbing fastness. The chelating agent, Ca2 +, Mg2 + and other metal ions can be added in the water to decrease the wet rubbing fastness. 2. Fabric can not be boiled with alkali soap after dyeing. Whether use mixed alkali fixation or single Na2CO3 fixation, the fabric must be fully washed with acetic acid 1 ~ 2mL / L in order to achieve fully hydrolysis of flooding, otherwise it will affect the effect of soap washing. 3. Control the quality of soap bo...